Thailand recycles well over 300,000 tonnes of PET bottles a year into flake, fibre and food-grade pellet, and every recycling extruder and most compounding extruders carry a vent port under vacuum. The vacuum pulls out of the melt what would otherwise become bubbles, hydrolysis and odour: moisture, residual monomer, degradation products and, in PET, cyclic oligomers that sublime at process temperature and condense as white wax on everything cooler. The pump on an extruder vent lives in the harshest vapour stream in the plastics industry, and most of the engineering is about keeping the oligomer out of it.

1. What the vent removes

At the vent zone the screw is designed to run partly filled, exposing the melt surface to the vacuum. From a PET recycling melt at 270–285 °C, the vent removes:

  • Water — flake dried to 50 ppm still carries moisture, undried flake 3,000–5,000 ppm. Water at these temperatures hydrolyses PET, cutting intrinsic viscosity (IV); the vent is what lets a recycler run with less pre-drying.
  • Acetaldehyde and other volatile degradation products — the "flavour" issue in food-grade PET; the vent removes most of it.
  • Cyclic trimer and other oligomers — 1–2 % of the PET mass is oligomer in equilibrium with the polymer; at 280 °C under vacuum a fraction sublimes. It deposits as a waxy solid at 100–200 °C.
  • Air entrained with the flake, and contaminant volatiles — label adhesive, residual drink, PVC traces releasing HCl.

Vent vacuum levels: 20–50 mbar for ordinary degassing and compounding; 5–20 mbar for high-IV food-grade recycling and for polyamide and polycarbonate; below 5 mbar on multi-vent decontamination extruders aiming at food-contact approval.

Why does the vent not just blow melt into the pump?

It does, when the vent is designed badly or the vacuum too deep for the screw. The melt in the vent zone foams as volatiles leave it; too much vacuum or too full a screw and the foam rises into the vent port — "vent flooding" — and polymer strands climb into the vacuum line. Vent design (a decompression zone, a vent stuffer screw to push melt back, the right vacuum level for the melt viscosity) keeps the melt in the barrel. The vacuum system's job is to handle what the vent should pass: vapour, not polymer. A knock-out pot with a sight glass at the vent catches the strands that come anyway, and tells the operator when the vent is flooding.

2. The vapour load and the pump size

The load is set by the throughput and the volatile content, and it is small in mass and large in volume. A 1,500 kg/h PET recycling extruder on flake at 1,000 ppm moisture after a crystalliser-dryer:

  • Water: 1,500 × 0.001 = 1.5 kg/h
  • Oligomer sublimation: ~0.1–0.3 % of throughput → up to 4 kg/h, most of which must be condensed before the pump
  • Acetaldehyde and others: < 0.5 kg/h
  • Air leakage into a 280 °C vent flange: 1–3 kg/h

At 20 mbar and 150 °C (after the vent line has cooled the gas somewhat), 1.5 kg/h of water vapour is about 150 m³/h and 2 kg/h of air about 100 m³/h. The vapour that reaches the pump — after an oligomer condenser — is of the order of 200–300 m³/h at 20 mbar, and the pump is sized to hold that pressure against it: an LT230-160V two-stage liquid ring pump at its 20 mbar point, or a DSI300 dry screw.

The pump is not sized on pump-down: the vent is a continuous open process at steady state, and start-up (pulling the vent line down) is not time-critical.

3. Liquid ring or dry screw

Two-stage liquid ring (LT Series) is the extruder vent pump of record, for a reason: the water ring washes oligomer and polymer dust out of the gas and discharges them with the seal water, the pump tolerates the slugs and strands that a flooded vent sends, and the seal water condenses the water vapour load. Its weakness is the 33 mbar ultimate at 20 °C seal water — at a Thai 32 °C seal water temperature the effective ultimate is 60 mbar and a 20 mbar vent setting is out of reach. So the LT is run with chilled seal water (a small chiller, 8–15 °C, which also improves the condensation) or with an air ejector on its inlet, which extends it to 10 mbar. For 5–20 mbar on a food-grade line, a liquid ring with ejector or a Roots booster ahead of the LT.

Dry screw (DSI Series) reaches 0.05 mbar without water, so any vent level is available, and the rotors run at 150–200 °C — hot enough that oligomer passes through as vapour rather than condensing in the pump, to be caught in a condenser on the exhaust side at atmospheric pressure, where a simple water-cooled trap does it. The dry screw costs more, uses no seal water (relevant where water discharge is regulated, which for a PET recycler with oligomer and acetaldehyde in the effluent increasingly it is), and needs the oligomer that does condense in its inlet line managed — heated inlet, cyclone, strainer. It does not tolerate polymer strands; the knock-out pot and a coarse strainer are mandatory.

The pattern in new Thai recycling lines: dry screw on the main vent of a food-grade line, liquid ring on compounding and fibre lines.

4. The oligomer trap

Whichever pump, the first element after the vent is an oligomer condenser — a water- or air-cooled vessel with a large cool surface (a tube bundle or baffles) at 60–90 °C where the cyclic trimer deposits, with access doors for cleaning. Design points:

  • Two in parallel, so one is cleaned (burned off at 300 °C or mechanically scraped) while the other runs; a 1,500 kg/h line fills a trap in days.
  • The vent line from barrel to trap heated above 250 °C so oligomer does not plate out in the pipe and choke it.
  • After the trap, a knock-out pot with sight glass and drain for water condensate and the fine oligomer mist, then the pump.
  • For a liquid ring pump, a seal water separator with a strainer and a skimmer, because oligomer floats.

Without the trap, an LT pump's seal water tank fills with wax in a week and a DSI's inlet strainer in a shift.

5. Solid-state polycondensation and decontamination

Food-grade recycling raises the IV of the pellet by solid-state polycondensation (SSP): pellets held at 200–220 °C for 8–15 hours under vacuum (0.5–2 mbar) or nitrogen, during which chain-extension reactions release ethylene glycol and water, and contaminants migrate out. The vacuum SSP reactor is a large batch duty: a 10–20 m³ vessel, pumped to 1 mbar and held against a load of glycol vapour and air leakage — a Roots booster on a dry screw (MB600 on a DSI300) with a glycol condenser between booster and backing pump. Oil-sealed pumps are a poor choice: glycol in the oil is permanent.

Decontamination extruders for food-contact approval run two or three vents in series at falling pressure, the last at 1–5 mbar; they are dry-screw duties, with a booster on the final vent.

6. A worked line

A 1,500 kg/h food-grade PET bottle-flake recycling line: crystalliser- dryer, twin-screw extruder with one vent at 15 mbar, melt filter, underwater pelletiser, SSP reactor 15 m³ at 1 mbar.

Duty Pressure Gas Dr.Vakuum answer
Extruder vent 15 mbar Water, oligomer, acetaldehyde, air Heated line → duplex oligomer traps → knock-out pot → DSI300 with exhaust condenser
Vent, alternative 15 mbar as above LT230-160V with chilled seal water and inlet air ejector
SSP reactor 1 mbar Glycol, water, air MB600 + glycol condenser + DSI300
Flake dryer (if vacuum type) 50 mbar Water LM200-065

Recommended Dr.Vakuum machines

Two-stage liquid ring (LT Series) — vents at 20–50 mbar, washes the oligomer out, tolerates flooding: LT185-080 (110 m³/h), LT200-120 (155 m³/h), LT230-160V, LT250-200 (525 m³/h).

Dry screw (DSI Series) — deep vents, no seal water, hot rotors pass oligomer: DSI150, DSI300, DSI630.

Roots boosters (MB Series) — SSP and decontamination vents: MB300, MB600.

The plant-wide vacuum for moulding machines downstream is a different duty — see Central vacuum system for an injection moulding facility.